How to Specify Tungsten Heavy Alloy on a Drawing: ASTM B777, AMS 7725, MIL-T-21014
October 27, 2026
How Much Does a Tungsten Ball Weigh? Sphere Weight by Diameter
November 10, 2026Is tungsten magnetic? Not in any way you would notice with a hand magnet. Pure tungsten is paramagnetic, which means it is attracted so weakly that a magnet will not pick it up. The answer changes for tungsten heavy alloy, the form most counterweights are made in, because the binder around the tungsten grains decides it. A nickel-iron binder makes the alloy slightly magnetic. A nickel-copper binder makes it nonmagnetic, which ASTM B777 defines as a maximum magnetic permeability of 1.05. If a counterweight is going near an MRI magnet, a magnetometer or a compass, that difference is the whole specification, so this guide covers how to choose it, how to write it down, and what can still go wrong.
Pure Tungsten Is Paramagnetic
Paramagnetic materials are drawn weakly toward a magnet only while it is close, and keep no magnetism afterward. Tungsten is one of them. It is not ferromagnetic the way iron, nickel and cobalt are, so a magnet will not stick to a pure tungsten rod or cube.
The effect is small enough to be useful. A 2015 paper from Indiana University on materials with low magnetic susceptibility for sensitive measurements mixed tungsten powder, which is paramagnetic, with bismuth, which is diamagnetic, so the two opposite responses cancel. That works because tungsten’s response is weak and predictable, and it shows how much very sensitive measurements care.
Tungsten Heavy Alloy: The Binder Decides
Heavy alloy is 90 to 97 percent tungsten, held together by a metal binder. Nickel and iron are ferromagnetic and copper is not, so the binder sets the magnetic behavior of the whole part.
| Binder | Magnetic behavior | ASTM B777 classes | Minimum tensile |
|---|---|---|---|
| Nickel-iron (W-Ni-Fe) | Slightly magnetic | 1 to 4 | 758, 758, 724 and 689 MPa |
| Nickel-copper (W-Ni-Cu) | Nonmagnetic | 1 to 3 only | 648 MPa |
Class 4 is magnetic only. At 97 percent tungsten there is not enough binder left to hold the copper system together at production strength. The class tensile figures are the ones in our ASTM B777 class breakdown. Nickel-iron is the more common choice and the stronger one, so nonmagnetic is a deliberate trade, not a default.
What Nonmagnetic Means on a Drawing
ASTM B777 says heavy alloys may contain elements that make them magnetic, and that freedom from magnetic response has to be stated in the purchase order. It defines nonmagnetic material as having a maximum magnetic permeability of 1.05, and it says Class 4 is not available in a nonmagnetic grade. These lines are from the 2007 edition of the standard. The current edition is B777-15, reapproved in 2026, so check its wording before you copy any of this.
Three details to pin down before you order:
- The number. Write the permeability limit on the drawing instead of just the word “nonmagnetic.”
- The test. The 2007 edition cites ASTM B193 for the measurement, but B193 is a resistivity method. ASTM’s method for weakly magnetic materials is A342, which has the user specify the field strength for some of its methods. Ask the supplier which method and field strength it uses.
- The proof. Ask for the measured value on the certificate of conformance.
A hand magnet cannot check any of this. A permeability of 1.05 and one of 1.00 look the same on a bench, so the limit has to be measured with an instrument.
The trade shows up in the strength numbers. Nonmagnetic Classes 1 to 3 carry a minimum tensile strength of 648 MPa, against 758 or 724 for the standard grades. In the 2007 edition the minimum elongation for nonmagnetic material also drops, to 2 percent for Classes 1 and 2 and 1 percent for Class 3, from 5 and 3. If the part sees shock or has thin sections, size it with those lower floors.
Where Nonmagnetic Counterweights Matter
The usual reasons are MRI equipment, shipboard compasses and sensitive instruments, anywhere a stray magnetic response would push a reading or pull on the part. Instruments that measure magnetic fields are the clearest case, since even small amounts of iron near the sensor show up as error. Our guide to counterweights and ballast covers why tungsten is chosen to put mass in a small space in the first place.
One caution for MRI work: nonmagnetic does not mean MR Safe. Under ASTM F2503, as summarized by the British Institute of Radiology, MR Safe labelling is only valid for items composed entirely of electrically nonconductive, nonmetallic and nonmagnetic materials. A tungsten counterweight is a conductive metal, so it cannot be MR Safe on its own however low its permeability is. Whether a part is acceptable in a given scanner is decided by the maker of the device it goes into, through its own MR safety testing.
What Can Still Make a Nonmagnetic Part Magnetic
A nickel-copper alloy can still fail a sensitive check, and the alloy is often not the cause.
- Plating. B777 allows coated parts, and a nickel coating can bring the magnetism back. Plating sources say electroless nickel with more than about 11 percent phosphorus is nonmagnetic, and that heat above roughly 625 °F can make it magnetic again, as this plating guide on electroless nickel magnetism explains. If a part needs a coating, state its composition and its condition, and have the permeability measured on the coated part.
- Iron picked up from tools and handling. Iron on a surface can read as magnetic even when the binder has none. Ask the supplier how it controls tooling and fixtures, and keep steel fasteners and fixtures away from the part in your own assembly.
- The wrong binder on the order. Say nickel-copper or nonmagnetic on the purchase order and confirm it on the certificate, so a nickel-iron lot never gets substituted.
How to Order Nonmagnetic Tungsten Heavy Alloy
- Cite ASTM B777 and a class from 1 to 3. Our guide to specifying heavy alloy on a drawing shows the full callout, including AMS 7725F.
- Write nonmagnetic, the permeability limit and the test method in the material note.
- State any coating and whether the magnetic limit applies after coating.
- Ask for the measured permeability on the certificate.
- Send the drawing through our quote form and say what instrument or device the part is for.
NONMAGNETIC: RELATIVE PERMEABILITY 1.05 MAX PER ASTM B777. TEST METHOD AND FIELD STRENGTH: ____. MEASURED VALUE ON CERTIFICATE.
Whatever the binder, a small heavy alloy part weighs more than it looks. USA Tungsten’s care and handling guide for tungsten bucking bars covers the same weight points for the same alloy family: keep a firm grip and set the part down instead of dropping it.
Frequently Asked Questions
Is tungsten magnetic?
Pure tungsten is paramagnetic, so it is only very weakly attracted to a magnet and a hand magnet will not pick it up. Tungsten heavy alloy depends on its binder: nickel-iron is slightly magnetic, and nickel-copper is nonmagnetic.
Will a magnet stick to tungsten?
Not to pure tungsten. A magnet may be slightly drawn to nickel-iron heavy alloy, and it will not respond to nickel-copper heavy alloy. A weak hand magnet cannot tell a nonmagnetic grade from a slightly magnetic one reliably, so use a measured permeability for anything that matters.
Is tungsten carbide magnetic?
It depends on the binder. Cemented carbide with a cobalt binder is more magnetic than grades with a nickel binder, according to patent literature, and nickel-bound grades are usually only weakly magnetic. If it matters, ask for the binder and a measured value. See this patent on nonmagnetic nickel tungsten carbide for the background.
Does tungsten block magnetic fields?
No. Shielding a magnetic field takes high-permeability materials, and tungsten is not one of them. Tungsten heavy alloy is used to shield X-rays and gamma rays, which is a different job.
Can tungsten counterweights be used near an MRI?
A nickel-copper alloy can be specified for a low magnetic response, but nonmagnetic does not make a part MR Safe. A tungsten counterweight is a conductive metal, so it is not MR Safe on its own, and the maker of the device it goes into decides whether it is acceptable in a given scanner.
Why is Class 4 not available as nonmagnetic?
At 97 percent tungsten, there is not enough binder to hold a nickel-copper system together at production strength. Class 4 is made with nickel-iron only, so it is slightly magnetic. Choose Class 1, 2 or 3 if the part has to be nonmagnetic.
How do I specify nonmagnetic tungsten heavy alloy?
Cite ASTM B777 with a Class 1, 2 or 3, write nonmagnetic with a permeability limit of 1.05 maximum and the test method, state any coating, and ask for the measured value on the certificate.
Tungsten Parts Wyoming manufactures tungsten and tungsten heavy alloy components, powder to finished part, in Laramie, Wyoming, under ISO 9001. Tell us the instrument or device your counterweight is for, and send the drawing through our quote form. Our tungsten heavy alloy page lists the grades, and full data by class is on our technical data page.